PPF Journal · Testing
How PPF yellowing is actually tested
Videos of film turning yellow under a lamp are everywhere. Here is what a real weathering test controls that a lamp video does not, how to read the number it produces, and what HAUT™ film measured.

By Vadim Nedelenko, founder of HAUT
· Updated
The short answer
A lamp video shows one sample under unknown conditions
A lamp video shows what happened to one piece of film, under one lamp of unknown spectrum and strength, at a temperature nobody measured. It cannot be repeated, and it cannot be compared with the next video.
A weathering test to ASTM G154 fixes the lamp, the light intensity, the temperature and the moisture, runs several specimens, and measures the color change with an instrument to ASTM E313. Run two films through the same cycle and you can compare them. That is the whole difference.
Side by side
Lamp video vs ASTM G154, Cycle 1
| What is controlled | Lamp video | ASTM G154 weathering test |
|---|---|---|
| Light source | Whatever lamp is on hand: a UV flashlight, a germicidal tube, a mercury curing lamp, a work light. Spectrum not stated. | UVA-340 fluorescent lamps, which closely match sunlight from 365 nm down to its ground-level cutoff at about 295 nm. |
| Irradiance | Unknown. Depends on the lamp, its age and how close it is held. | Controlled: 0.89 W/m²/nm at 340 nm in Cycle 1, held by the chamber's own sensors. |
| Temperature | Not measured. A lamp close to the film can heat it far beyond what the light alone would do. | 60 °C (140 °F) during the UV phase, 50 °C (122 °F) during condensation, measured on a black panel. |
| Moisture | None, or a spray bottle. | 4 hours of condensation in every 12-hour cycle, the way dew sits on a car overnight. |
| Samples | One piece of film, run once. | Several specimens of the same film, with an unexposed piece kept as the reference. |
| How the result is read | By eye, on camera, under whatever light the room has. | Yellowness index measured with an instrument per ASTM E313, before and after. |
| Can someone else repeat it? | No. Change the lamp or the distance and you get a different video. | Yes, to a written method. For a fair comparison, run both films in the same chamber at the same time. |
What a lamp cannot show
Four things to know before you trust a video
Most lamps in these videos emit UV that never reaches a car
UV comes in three bands: UV-C (100–280 nm), UV-B (280–315 nm) and UV-A (315–400 nm). The atmosphere absorbs all of the UV-C and most of the UV-B, so sunlight at ground level stops at about 295 nm, and roughly 95% of the UV that reaches a car is UV-A. A germicidal tube emits UV-C at 254 nm. A mercury curing lamp, the kind used on industrial coatings and screen-printing ink, puts out UV-C, UV-B, UV-A and a lot of heat. UV shorter than 295 nm carries more energy and can start reactions in the polyurethane, top coat and adhesive that sunlight on a car does not. So a film can yellow under one of these lamps and stay clear on a car, and two films can rank in a different order under it than they do outdoors.
Beading is not UV resistance
Water beading is the top coat's surface energy. Yellowing resistance lives in the polyurethane, the UV stabilizers and the adhesive. A film can do one well and the other badly.
Heat changes the result
A lamp held close heats the film as well as lighting it. A black hood in summer sun gets hot too, but a test that does not measure temperature cannot tell you whether you are watching UV damage or heat damage.
Yellowing has more than one source
Quality clear PPF uses aliphatic polyurethane, because aromatic polyurethane yellows in sunlight. The adhesive matters too: an automotive adhesive is crosslinked to hold for years and release cleanly, and a close lamp hits it with heat and short-wave light a car never sees. If it reacts, you're watching a lamp effect, not sun damage. Passing or failing a lamp test tells you about the lamp, not the install.
HAUT's numbers
What HAUT film measured after 500 to 2,000 hours
ASTM G154 Cycle 1 (UVA-340, 8 h UV at 60 °C (140 °F) / 4 h condensation at 50 °C (122 °F)), three specimens per film. ΔYI is the change in yellowness index per ASTM E313 against the same film before exposure: lower is better.
Master
| Exposure | ΔYI | Gloss retained |
|---|---|---|
| 500 h | 0.49 | 99.0 % |
| 1,000 h | 0.88 | 97.9 % |
| 1,500 h | 1.26 | 96.5 % |
Master Plus
| Exposure | ΔYI | Gloss retained |
|---|---|---|
| 500 h | 0.44 | 99.2 % |
| 1,000 h | 0.81 | 98.2 % |
| 1,500 h | 1.15 | 97.1 % |
| 2,000 h | 1.54 | 95.8 % |
Mist (satin)
| Exposure | ΔYI | Sheen shift |
|---|---|---|
| 500 h | 0.51 | −0.3 GU |
| 1,000 h | 0.92 | −0.8 GU |
| 1,500 h | 1.31 | −1.3 GU |
No cracking, blistering or delamination at the final reading on any of the three. UV weathering values: qualification testing of the US production line (qualification lots May 2025), performed by the manufacturer’s QA laboratory, three specimens per film.
For any brand
How to read a weathering claim
- The method and cycle are named. “ASTM G154 Cycle 1” is a claim you can check. “UV tested” is not.
- The hours are stated. 500 hours and 2,000 hours are different tests.
- The result is a measured number. A change in yellowness index per ASTM E313, not “no visible yellowing”.
- Who tested it, and how many samples. A sheet should say whose laboratory ran the test and on how many specimens.
- Compare like with like. Two films are comparable only on the same cycle at the same hours.
More on every method we publish against, and what each number means on a car, is on film technology and test methods.
Questions about UV tests
Because a lamp tests how a film reacts to that lamp, not to the sun. Several things decide it, and none of them is “which film lasts longer on a car”:
- Wavelength. UV absorbers in PPF are built for sunlight at ground level. A germicidal or mercury curing lamp puts out shorter-wave UV that never reaches the road, and different top coat and adhesive chemistries react to it very differently.
- Heat. The center of a lamp's beam runs hotter than the edges. Two samples a few inches apart don't see the same temperature.
- Adhesive. Some adhesives react to close, hot, short-wave light faster than others. On a white card that reads as “yellow film.”
- The samples themselves. Roll age, storage, cap sheet on or off, thickness — none of it is shown on camera.
So a side-by-side lamp video shows which film reacts to that lamp. For a comparison that means something on a car, run both films through the same G154 cycle with the same lamps for the same number of hours and compare the measured change in yellowness index.
We spent six years installing HAUT film on customer cars through a closed network of partner shops before selling a single roll—and we still install it daily in our New Jersey flagship studio, with zero warranty yellowing claims.
Tested film, installed by certified shops
HAUT film is installed only by certified shops, and carries a 10-year warranty that covers premature yellowing.